The part keeps burning — why does the adjustment only work for a while?

1970.01.01

The part keeps burning — why does the adjustment only work for a while?

The usual scene is a small fire drill. A corner goes dark again, the setter eases off injection speed and drops the melt temperature a little, checks a few parts, and it is fine. Everyone moves on. A while later the same corner burns again. Slow it a little more, fine again. The cycle repeats until somebody asks whether the part can be made at all.

Whether the part can be made and whether the air has somewhere to go are two different questions. Burning is trapped air: air in the cavity and gas released by the melt cannot escape, are compressed and heated, and scorch the flow front. The material has not suddenly gone bad and the press has not suddenly disobeyed. Gas stuck in that spot is the cause.

One step is often skipped before touching anything: confirming that this actually is trapped air. A burn normally sits at the end of fill, at a weld line or in a deep pocket, shaped like a scorched band, in a repeatable place. Some black specks are not that at all — material carbonised after sitting too long in the barrel, poorly dispersed masterbatch, or contamination in the feed. Those specks scatter across the part with no fixed address, and shift when the material batch changes or the barrel is purged. The two look alike but call for opposite remedies: one is gas with no route out and needs a change to the tool; the other is a material condition and needs the material and process addressed. Mix them up and you will spend effort venting a tool that is fine, or keep adjusting the material while ignoring the corner that is blocked. Asking whether the mark has a pattern is the cheapest triage there is.

Why does slowing down and cooling down work? Because it gives the gas more time to find a way out through the gaps and reduces how hard it is compressed. The symptom eases, certainly. But something is paid for it: cycle time stretches, the flow end may start to look dull at a lower melt temperature, the weld line reads more strongly, and chasing the burn through packing changes drags dimensions about. The burn is suppressed for now and the cost is spread into cycle, appearance and stability. Worse, the adjustment hides the signal — what should have stopped the line for a vent check is papered over with parameters, and the fault comes back.

Venting is not something to leave as "as usual". It has to be worked out in three places: the end of fill, where the melt fronts meet at a weld line, and the bottom of a deep pocket. The first two are where air is most easily sealed off by the advancing front; the third is a corner air cannot readily leave on its own. Without a path in those places, the gas waits for one particular shot in one particular moment — which is why burning looks irregular: not every shot, just an occasional one, and often right when the press is being pushed. That occasional quality is gas hovering at a threshold.

The vent itself needs thought. Too shallow and it does nothing; too deep and material flashes, leaving a deflashing operation behind. The right position with insufficient width still will not breathe. And it is machined, so what is drawn and what is cut differ slightly — that slight difference is often the answer to "why is it still burning after we vented it". In production the vent slowly fills with release-agent residue and deposits: a new tool runs clean, an older one burns, and that is usually why. Unlike a parameter it cannot be changed on a screen; touching it means stopping, stripping and machining, so the floor would rather adjust again than stop and clean.

Material adds to it. A conventional compound gives off relatively modest gas; glass-fibre reinforced and flame-retardant grades release decomposition gas far more actively at temperature. The same tool can change where and how it burns with a new batch or a different masterbatch. That is the real reason behind "this setting worked last time": the setting did not change, the material did, and the gas load with it. Keep a note of each episode — which material, which location, what was adjusted, whether the vent was cleaned — and after a few rounds you can see what came from the material and what came from an inadequate path in the tool.

Trial is also the chance to check whether venting is adequate, long before production turns it into a fire drill. Watch the filling rather than only the finished part: run at a lower speed and see whether the front stalls as it reaches the end, whether the weld line darkens as the fronts meet, whether the deep pocket fills only at the last moment. A short-shot study helps — stop at successive stages of fill and see where the gas begins to be sealed in. Once the cavity is full, that evidence is gone; all you have left is a scorch mark to guess from. Putting a vent check on the trial list is far cheaper than sorting it out by trial and error in production. It also answers a second question: whether this spot is short of venting, or whether filling and packing were never right in the first place.

So the order matters: locate first, change steel second, adjust parameters last. Locating means looking at where the burn sits — end of fill, weld line or deep pocket — because the location is the clue. Changing steel means putting a vent where it belongs, adding a vent insert where needed, giving the gas a route out. Only then do parameters come in for fine tuning, to settle the window rather than plug a hole in the design. Do it the other way round and you get the fire drill: adjust until there is nothing left to adjust, suspect the tool, and only at the end remember the vent.

In production, venting is not a one-off job. It blocks, it dulls, it fills gradually with residue. Put vent cleaning into the maintenance schedule alongside the cooling channels and guides, and on a burn check the vent before touching parameters. Reverse that order and the cost is different in kind — cleaning on schedule is a planned stop, while repeated adjusting, repeated scrap and the occasional mark the customer finds are not.

In the end, burning is not a failure of setting skill; it is air trapped by a drawing. Parameters can suppress a burn but cannot give the gas a way out. Jingmu records the burn location and the corresponding venting action in the trial issue list, so that a temporary fix becomes a one-time solution.